TC4 titanium alloy is a typical α+β two‑phase titanium alloy. Thanks to its excellent specific strength, corrosion resistance, biocompatibility and other characteristics, it is widely used in aerospace, automobile manufacturing, biomedical and many other fields. Forging is a key step in its forming process. By adjusting the deformation temperature, deformation amount and heat treatment schedule, the morphology, size and distribution of the α phase and β phase in the microstructure can be remarkably modified, which further affects the tensile properties of the material, such as tensile strength, yield strength and elongation. This paper carries out a systematic study from three aspects: the regulation mechanism of microstructure by forging process, the correlation between microstructure and tensile properties, and the collaborative optimization of process parameters. It aims to reveal the intrinsic relationship among forging process, microstructure evolution and property response, so as to provide a theoretical basis for the precise design of forging processes for TC4 titanium alloy.
TC4 titanium alloy should be forged strictly either in the α+β two‑phase region (below \(T_\beta\), and \(T_\beta\) is generally about 980–1000 ℃) or in the β single‑phase region (above \(T_\beta\)). Deformation in different phase regions leads to fundamentally different microstructure features. When deformed in the α+β two‑phase region, the difference in slip systems between the α phase (HCP structure) and the β phase (BCC structure) (approximately 12 slip systems for α phase and 48 for β phase) results in incompatible deformation. Specifically, the α phase forms equiaxed grains via dynamic recrystallization with grain sizes generally ranging from 1 to 5 μm, while the β phase is elongated into bands along the deformation direction, with band widths of 2–8 μm. When the deformation temperature approaches \(T_\beta\), the volume fraction of the β phase increases markedly from the initial 30%–40% to 60%–70%, the α phase gradually dissolves, and lamellar α phase increases in the microstructure, forming basket‑weave or Widmanstätten features. The thickness of lamellar α phase is 0.1–0.5 μm. If deformation is performed in the β single‑phase region, the prior β grains grow rapidly at high temperature. For deformation at 1050–1100 ℃, the prior β grain size can increase from the initial 50–100 μm to 200–500 μm, forming coarse β grains after deformation. During cooling, the α phase precipitates along β grain boundaries or within grains, producing typical Widmanstätten microstructure characterized by network‑distributed grain‑boundary α phase and intragranular lamellar α phase. The width of grain‑boundary α phase is 1–3 μm, and the interlamellar spacing of intragranular lamellar α phase is 2–6 μm.
Deformation amount affects microstructure refinement by altering dislocation density and recrystallization degree. For deformation in the two‑phase region, an appropriate increase in deformation amount promotes dynamic recrystallization of the α phase. At the early deformation stage with a deformation amount of 10%–20%, dislocations pile up at α phase grain boundaries and α/β interfaces to form high‑density dislocation zones, where the dislocation density can reach \(10^7\)–\(10^8\ \mathrm{cm^{-2}}\). As the deformation amount increases continuously to 30%–50%, dislocations rearrange to form subgrain boundaries and eventually evolve into equiaxed α grains, which can be refined to 0.5–3 μm. Meanwhile, slip and twinning occur in the β phase during deformation, and a large number of dislocation walls form inside it with a spacing of 0.2–1 μm. These dislocation walls provide nucleation sites for subsequent recrystallization.
Heat treatment further adjusts the microstructure by controlling phase transformation, eliminating forging defects and optimizing material properties. A double annealing schedule, e.g. 900 ℃ × 1 h / AC + 600 ℃ × 4 h / AC, enables spheroidization of the α phase in the as‑forged microstructure. The first annealing step promotes partial dissolution of the α phase, and the second step drives spheroidization of the residual α phase via surface energy reduction, reducing the thickness of lamellar α phase and increasing the volume fraction of the β phase. The solution temperature exerts a significant influence on the content of primary α phase. For solution treatment in the α+β phase region, such as 950 ℃, partial dissolution of primary α phase occurs and the size of residual α phase decreases. For solution treatment in the β phase region, such as 980 ℃, the primary α phase dissolves completely, and basket‑weave α colonies form after cooling, whose size depends on the cooling rate.
Equiaxed microstructure consists of equiaxed α phase and intergranular β phase. It is characterized by relatively uniform α grain size (usually less than 5 μm) and strong interfacial bonding. During tensile loading, equiaxed α phase absorbs energy through coordinated deformation: slip systems activate inside grains, and deformation compatibility is realized via dislocation pile‑up and transmission at grain boundaries. The intergranular β phase, as a ductile phase, hinders crack propagation, which endows the material with high elongation (>15%) and reduction of area (>30%). Equiaxed microstructure shows low anisotropy, with the difference in tensile properties in different directions less than 10%, so it is suitable for components requiring complex forming (such as aero‑engine blades). Nevertheless, its strength is generally lower than that of lamellar microstructure owing to the lack of strengthening from lamellar phases. Equiaxed α grain boundaries tend to become crack initiation sites, and the strengthening effect of β phase is limited.
Mixed microstructure is composed of equiaxed α phase, secondary α phase and β phase. It is obtained by combining two‑phase‑region forging with double annealing. The equiaxed α phase, with a volume fraction of 30%–50%, provides plasticity for the mixed microstructure; the secondary α phase, thinner than 1 μm, improves strength by blocking dislocation motion; the β phase, with a volume fraction of 10%–20%, acts as a ductile phase to coordinate deformation. In tension, uniform plastic deformation firstly takes place in equiaxed α phase, secondary α phase impedes dislocation motion via the Orowan strengthening mechanism, and the β phase absorbs energy through the transformation‑induced plasticity (TRIP) effect. This mixed microstructure achieves a better strength‑ductility match than single equiaxed or lamellar microstructure, with tensile strength higher than 1000 MPa and elongation greater than 10%. It is especially suitable for aerospace components demanding excellent comprehensive mechanical properties, such as landing gears. The fraction of each phase in mixed microstructure can be precisely controlled by adjusting forging temperature and heat treatment schedule: increasing the forging temperature raises the content of secondary α phase, while lowering the forging temperature retains more equiaxed α phase.
The matching of deformation temperature and deformation amount should consider both microstructure refinement and dynamic recrystallization. For two‑phase‑region forging, a relatively low temperature (e.g. \(T_\beta-60\) ℃) combined with a moderate deformation amount (30%–50%) can produce fine equiaxed microstructure. At low temperature, the deformation resistance is relatively high, but the driving force for dynamic recrystallization is large, which favors fine grain formation. Meanwhile, moderate deformation amount promotes full recrystallization and avoids residual deformed microstructure. A higher temperature (e.g. \(T_\beta-20\) ℃) together with a large deformation amount (>50%) leads to mixed microstructure. At high temperature, the volume fraction of β phase increases, and large deformation facilitates the precipitation of secondary α phase while preserving part of equiaxed α phase. For β single‑phase‑region forging, the deformation amount must be strictly controlled (<30%) to prevent excessive grain growth, and subsequent heat treatment such as near‑β annealing is usually required to refine the microstructure. Equipment capacity also needs to be considered: although high temperature reduces deformation resistance, oxidation should be avoided; low temperature requires higher‑tonnage forging equipment.
Heat treatment schedules should be tailored according to forging processes and property requirements. For forgings forged in the two‑phase region, double annealing optimizes the proportion of equiaxed α phase and β phase. The first annealing temperature of 900–950 ℃ controls the content of primary α phase, and the second annealing temperature of 550–650 ℃ regulates the precipitation of secondary α phase. For β single‑phase‑region forgings, a near‑β annealing schedule such as 945 ℃ × 150 min + 985 ℃ × 25 min / air cooling is adopted to eliminate coarse Widmanstätten microstructure. The material is held in the β phase region to fully dissolve α phase, then rapidly cooled into the two‑phase region to promote uniform α precipitation, and finally aged to precipitate secondary α phase. The solution temperature is adjusted according to the primary α content: subcritical solution at 950 ℃ is used to retain primary α phase, and supercritical solution at 980 ℃ is used to eliminate primary α phase completely. The aging time controls the size of secondary α phase: short aging for 2 h generates fine secondary α phase, while long aging for 8 h causes coarsening of secondary α phase and strength degradation.
By adjusting deformation temperature, deformation amount and heat treatment schedule, the forging process of TC4 titanium alloy enables precise microstructure design and further optimizes tensile properties. Equiaxed microstructure features high plasticity and is suitable for complex‑formed components; mixed microstructure balances strength and ductility to meet the comprehensive performance requirements of high‑end equipment; lamellar microstructure is characterized by high strength, while its anisotropy needs to be addressed. Synergistic optimization of forging parameters requires comprehensive consideration of microstructure refinement, dynamic recrystallization and phase transformation. Specifically, the matching of deformation temperature and deformation amount balances microstructure refinement and equipment capacity, and heat treatment schedules are customized for specific forging routes. Multi‑fire forging and process integration can further improve microstructure homogeneity.