Large crankshafts, as the core load‑transfer components of power equipment, are subjected to alternating and impact loads, which impose stringent requirements on the comprehensive mechanical properties (matching of strength, toughness and hardness) of materials. Containing alloying elements such as Cr, Mo and V, 30CrMoV9 steel possesses good hardenability and tempering stability, making it a preferred material for manufacturing large crankshaft forgings. Its final performance is mainly determined by the quenching and tempering process (quenching + tempering): quenching governs the uniformity of martensitic microstructure, while tempering achieves the balance between strength and toughness by regulating microstructure transformation. The study reveals that tempering at 625 ℃ achieves strength‑toughness balance, and the comprehensive properties fully satisfy the technical specifications of a certain type of large crankshaft forging. This tempering condition can be adopted as the optimal quenching and tempering process for such forgings.
30CrMoV9 round steel is selected for the production of a specific type of large crankshaft forging. The round steel has a diameter of φ355 mm and a length of 4000 mm. It is produced via vacuum melting plus refining, followed by forging into round bars with a forging ratio greater than 4. Slow cooling is performed after forging. Upon delivery, the austenite grain size at the 1/2 radius position of the round steel shall be Grade 5 or finer. The chemical composition of the round steel is shown in Table 1.
Table 1 Chemical Composition of 30CrMoV9 (wt.%)
Production process of crankshaft forgings: incoming reinspection of round steel → heating to 1080 ℃ with holding for 3.5–5.5 h → die forging → trimming → quenching and tempering → sampling and inspection of finished products. Three sets of quenching-and-tempering schedules were tested.
Scheme 1: Charging into furnace at ≤650 ℃ → heating up to 880 ℃ and holding for 5 h → water quenching (exit water temperature 80–100 ℃) → tempering at 590 ℃ with holding for 9 h → air cooling out of furnace.
Scheme 2: The quenching procedure is identical to Scheme 1 → tempering at 625 ℃ with holding for 9 h → air cooling out of furnace.
Scheme 3: The quenching procedure is identical to Scheme 1 → tempering at 640 ℃ with holding for 9 h → air cooling out of furnace.
After air cooling to room temperature following tempering, longitudinal specimens were taken from both ends of the crankshaft for physical and chemical tests including room-temperature tensile test, impact test, microstructure observation and hardness measurement.
Comparative analysis of the three groups of physical and chemical properties shows that adjusting the tempering temperature under identical quenching conditions yields a remarkable improvement in comprehensive properties. For Scheme 1 with tempering at 590 ℃ (Table 2), the tensile strength ranges from 1066 to 1075 MPa, the hardness is 311.8–328 HBW, and the impact toughness is 56.52–59.71 J/cm². For Scheme 2 (Table 3), 625 ℃ is selected as the tempering temperature based on the trade-off of data from Scheme 1 and Scheme 3. Its tensile strength is 881–902 MPa, hardness 277.5–278.6 HBW, and impact toughness 103–105 J/cm²; the comprehensive properties meet the technical requirements of the product. Scheme 3 adopts tempering at 640 ℃ (Table 4), with tensile strength 825–834 MPa, hardness 259.2–261.6 HBW and impact toughness 200.6–206.6 J/cm². The ductility is greatly improved, yet its comprehensive properties fail to satisfy the product specifications.
Table 2 Test Results of Physical and Chemical Properties for Scheme 1 (Tempered at 590 ℃)
Table 3 Test Results of Physical and Chemical Properties for Scheme 2 (Tempered at 625 ℃)
Table 4Test Results of Physical and Chemical Properties for Scheme 3 (Tempered at 640 ℃)
It can be clearly seen from the comparison that under identical quenching conditions, higher tempering temperature leads to better ductility accompanied by decreased strength and hardness. The microstructures obtained by the three tempering processes are dominated by tempered sorbite. As the tempering temperature rises, carbides transform from fine clusters into coarse connected sheets. The residual lath martensite in the matrix tends to transform into equiaxed ferrite, and the precipitation of carbides from retained austenite increases. The properties follow the trend of “decreasing strength and hardness, increasing ductility and toughness”. Among them, the tempering process at 625 ℃ achieves strength‑toughness balance, with tensile strength of 881–902 MPa, impact toughness of 103–105 J/cm² and Brinell hardness of 277.5–278.6 HBW, satisfying the technical requirements on comprehensive properties for large crankshaft forgings.
Specimens of 20 mm × 20 mm were taken from the three heat‑treated products for metallographic examination. The test results are shown in Figure 1, Figure 2 and Figure 3.
Figure 1 Microstructure after Tempering at 590 ℃
Figure 2 Microstructure after Tempering at 625 ℃
Figure 3 Microstructure after Tempering at 640 ℃
Under the three tempering temperatures, the microstructure of 30CrMoV9 steel is predominantly tempered sorbite, consisting of equiaxed ferrite and dispersed carbides. However, obvious differences exist in the morphology, quantity of carbides and matrix state. The detailed characteristics are as follows.
(1) Scheme 1 (Tempered at 590 ℃) Tempering at 590 ℃ is a medium‑temperature tempering process. The diffusion capacity of carbon atoms is relatively weak at this temperature: martensite decomposition is incomplete, and partial lath martensite features remain. The amount of precipitated carbides is low, and these carbides are dispersed in the matrix in the form of fine clusters. The fine clustered carbides provide strong dispersion strengthening for the matrix, and the retained lath martensite also increases the strength of the material. Therefore, Scheme 1 achieves the highest strength and hardness. Nevertheless, the high dispersion of carbides and abundant residual martensite induce stress concentration, resulting in poor ductility and toughness.
(2) Scheme 2 (Tempered at 625 ℃) Tempering at 625 ℃ falls into the medium‑high temperature tempering range. The diffusion capacity of carbon atoms is greatly enhanced. The features of lath martensite almost disappear, and the matrix is fully transformed into equiaxed ferrite. The fine carbides precipitated at an earlier stage aggregate and grow up, with increased quantity and regular morphology (short rod‑shaped or granular), uniformly distributed in the equiaxed ferrite matrix. Equiaxed ferrite relieves stress concentration and improves ductility; the aggregated and coarsened carbides still maintain a certain dispersion strengthening effect. Consequently, Scheme 2 realizes the balance of “hardness‑ductility‑toughness” and meets the comprehensive property requirements of large crankshafts.
(3) Scheme 3 (Tempered at 640 ℃) Tempering at 640 ℃ is high‑temperature tempering with sufficient carbon atom diffusion. The original martensite orientation features vanish completely, and the matrix is composed of fully equiaxed ferrite. Carbides further aggregate, re‑dissolve and grow into coarse connected sheets with slightly reduced distribution uniformity. In addition, part of the carbon and alloying elements such as Cr and Mo dissolve into the matrix at high temperature, which may form a small amount of reverse‑transformed austenite and further improve ductility and toughness. However, carbide coarsening drastically weakens the dispersion strengthening effect, so Scheme 3 exhibits the lowest strength and hardness.
For large crankshaft forgings of 30CrMoV9 steel under identical quenching conditions, the tempering temperature plays a decisive role in microstructure and properties. As the tempering temperature increases, carbides in the microstructure evolve from fine clusters into coarse connected sheets, and the matrix transforms from residual lath martensite to fully equiaxed ferrite. The properties follow the rule that strength and hardness decrease while ductility and toughness increase.
Although Scheme 1 (tempered at 590 ℃) delivers the highest strength and hardness (tensile strength: 1066–1075 MPa, Brinell hardness: 311.8–328 HBW), it has the lowest impact toughness (56.52–59.71 J/cm²) and poor ductility, so it cannot withstand impact loads.
Scheme 2 (tempered at 625 ℃) achieves strength‑toughness balance. Its tensile strength is 881–902 MPa, impact toughness reaches 103–105 J/cm², and hardness is 277.5–278.6 HBW. The comprehensive properties fully satisfy the technical requirements of a certain type of large crankshaft forging, and this tempering process can be adopted as the optimal quenching and tempering process for such forgings.
Scheme 3 (tempered at 640 ℃) possesses the best ductility and toughness (impact toughness: 200.6–206.6 J/cm²), yet its strength and hardness are insufficient (tensile strength: 825–834 MPa, hardness: 259.2–261.6 HBW), failing to meet the load‑bearing requirements.